Technology Study of Comprehensive Recovery of Multi Metals from Waste Catalyst
Received:December 01, 2013   Revised:December 03, 2013   Accepted:December 04, 2013      Published Online:June 23, 2014
View Full Text  View/Add Comment  Download reader
DOI:10.3969/j.issn.1007-7545.2014.07.011
KeyWord:waste catalyst; W; Mo; V; comprehensive recovery
           
AuthorInstitution
ZHU Lai-dong 西北矿冶研究院
LU Xing-wu 西北矿冶研究院
YI Chao 西北矿冶研究院
HE Guo-cai 西北矿冶研究院
Hits: 4027
Download times: 4956
Abstract:
      Tungsten, molybdenum, and vanadium were comprehensively recovered from waste catalyst with a series of processes including two-stage countercurrent leaching, vanadium precipitation, recrystallization after ammonia dissolving, and purification. The results show that leaching rate of W, Mo, V is all 95% above, and comprehensive recovery is over 90% under the optimum conditions including leaching temperature of 70 ℃, leaching time of 3.5 h, sodium carbonate concentration of 350 g/L, and ratio of liquid to solid of 3∶1.
Close