Recovery of Rhodium from Rhodium-bearing Solution by DETA Precipitation |
Received:April 24, 2018 Revised:May 03, 2018 |
View Full Text View/Add Comment Download reader |
DOI:doi:10.3969/j.issn.1007-7545.2018.09.012 |
KeyWord:DETA; rhodium; recovery |
Author | Institution |
ZHAO Yu |
贵研资源(易门)有限公司 |
WU Xilong |
贵研资源(易门)有限公司 |
HE Xiaotang |
贵研资源(易门)有限公司 |
XIONG Qingfeng |
贵研资源(易门)有限公司 |
WANG Huan |
贵研资源(易门)有限公司 |
LI Yong |
贵研资源(易门)有限公司 |
WANG Jinying |
贵研资源(易门)有限公司 |
|
Hits: 970 |
Download times: 767 |
Abstract: |
The process to recover rhodium from rhodium-bearing solution by DETA precipitation method was studied. Rhodium precipitation is in a steady state when reaction temperature is 100 ℃ and dosage of DETA solution is 200 mL for 1 500 mL rhodium-bearing solution. Rhodium powder with purity of 99.9% above is obtained with rhodium direct recovery of 96.77% after calcining and reduction. |